The microstructural changes of Φ20 mm×5 mm polymer bonded explosives (PBX) sample based on HMX pressed at 50-250 MPa were investigated by scanning electron microscopy(SEM). The particle size distributions of HMX were measured by laser particle size analyzer. Results show that as the porosity in samples reduces, the crystal twinning and cracking in pressed PBX increases obviously. The mean particle diameters of HMX is 34.37 μm before being pressed, and after being pressed under 50,100,250 MPa, the mean particle diameters of HMX are 31.16 μm , 27.90 μm and 26.37 μm, respectively.
Reference
Related
Cited by
0
Article Metrics
PDF:
HTML:
Abstract:
Cited by:
Get Citation
梁华琼,周旭辉,唐常良,等. HMX钢模压制的微观结构演变研究[J].含能材料,2008,16(2):188-190. LIANG Hua-qiong, ZHOU Xu-hui, TANG Chang-liang, et al. Microstructural Evolution of HMX During Pressing[J]. Chinese Journal of Energetic Materials,2008,16(2):188-190.